- We have added this recipe
to our report on the Floating Blue, which goes a
little against the philosophy of this type of glaze
which matures normally at C/6, but that shows that it
is necessary to stray from the beaten track. As any
very good "Floating Blue" this recipe contains boron,
rutile and a sodic feldspar/feldspathoid (In the case
of C/6 recipes, it is Nephelite Syenite that plays the
role of the sodic
feldspar/feldspathoid).
-
- Edouard
Bastarache
-
-
-
-

- Oeuvre
réalisée par Jean Marc
Ringuette
-
-
- Here is the
real recipe that can be used in North America
:
-
-
|
Bass C/04
Floating Blue
|
|
Sodium/calcium
Feldspar (Kona F-4) (may be replaced by
CR-79)
|
23
|
|
Gerstley
Borate
|
23
|
|
Ferro frit #3134
|
23
|
|
Silica
|
8
|
|
Zinc oxide
(Calcined)
|
7
|
|
Kaolin
(Calcined)
|
14
|
|
Rutile
|
4
|
|
Red Iron
Oxide
|
2
|
|
Cobalt
Carbonate
|
1.5
|
-
- Given the absence of
Gerstley Borate in the "old Europe", here is the
substitution which I propose to our friends on the
other side of the pond :
-
- Bass C/04
Floating Blue substituted recipe for Europe :
-
-
|
Bass C/04
Floating Blue - Subsituted recipe for
Europe
|
|
Soda Spar
|
12
|
|
Ferro frit
#3134
|
46
|
|
Dolomite
|
5
|
|
Zinc Oxide
(Calcined)
|
7
|
|
Kaolin
|
10
|
|
Kaolin
(Calcined)
|
11
|
|
Silica
|
7
|
|
Rutile
|
4
|
|
Red Iron
Oxide
|
2
|
|
Cobalt
Carbonate
|
1.5
|
-
-
- Seger Formula :
-
-
|
KNaO
0.200
|
Al2O3
0.280
|
SiO2
1.95
|
|
CaO
0.500
|
|
MgO
0.070
|
B2O3
0.390
|
|
ZnO
0.220
|
-
-
-
-
-
-
|
|
- Edouard
Bastarache M.D.
- (Occupational
& Environmental
Medicine)
-
- Author
of " Substitutions for raw ceramic
materials "
- Tracy,
Québec, CANADA
- edouardb@colba.net
|
-
-
- Smart2000.fr
©
Avril 2005
-
FRANCE
- Écrit
et documenté par le propriétaire du site
// Contact : Smart2000@wanadoo.fr
- Document
pour CONSULTATION PRIVÉE uniquement - Toute
reproduction totale ou partielle est
interdite
-
-
-
-
- Smart2000.fr
le site
dédié aux passionnés de
céramique
-
- Smart2000
- FRANCE sur https://smart2000.fr/
-
- This
entire page Copyright © 2005-2023, All Rights
Reserved.
- Les textes et
les photos restent la propriété de leur
auteurs, ils ne peuvent être
réutilisés sans un accord
préalable. Nous consulter.
|